A DFM review is not a courtesy. On a typical enclosure it is the difference between a two-plate tool with a straight pull and a tool with two slides, a lifter and a heated sprue. Here is the list our engineers work through before a moulding number goes out, in the order the problems usually appear.
1–2. Wall thickness and uniformity
Nominal wall drives everything downstream: fill pressure, cycle time, warp, sink. For ABS and PC-ABS, 1.8–2.5 mm is comfortable; for PP, 1.2–2.0 mm; for PC, 2.0–3.0 mm. More important than the nominal value is uniformity — keep variation within ±15% across the part. A 3 mm boss on a 2 mm wall will sink on the far face, every time.
3. Draft on every vertical face
1–2° on smooth surfaces, 2–3° on textured ones (add roughly 1° per 0.025 mm of texture depth). Zero draft means the part drags, scuffs and sometimes stays in the cavity. This is the single most common omission in customer CAD.
4. Radii, not sharp corners
Inside corners should carry a radius of at least half the wall thickness — 0.5 mm minimum, 1 mm preferred. Sharp internal corners concentrate stress and are hard to fill; sharp external corners are fragile and chip.
5. Ribs: thickness and spacing
Rib thickness at 50–60% of the adjacent wall avoids sink. Spacing should be at least 2× wall thickness, and rib height should stay under 3× wall thickness unless you add a gusset. Deep, thin ribs need a taller tool and a slower fill.
6. Bosses
Boss wall 50–60% of the main wall, outside diameter around 2× the screw diameter, and a radius at the base. Isolate the boss with a shallow groove or a thinner web so it does not pull a sink mark on the cosmetic face.
7. Gate location and witness
Where the plastic enters decides the weld lines, the orientation and the cosmetic defect you will live with. Tell us where the gate is allowed to show. A hidden gate costs tooling money; a gate on a visible face costs a customer.
8. Undercuts and side actions
Every undercut is a slide, a lifter or a split. Each adds tooling cost and maintenance. Snap fits and living hinges are legitimate — but they need to be designed as such, with the right material and a relief that lets the steel move.
9. Tolerances that respect shrinkage
Moulded parts shrink 0.4–0.8% depending on resin and fill, and shrink is not uniform in three directions. Do not tolerance a moulded dimension tighter than the resin datasheet supports; use the moulding tolerance table (±0.1 mm on small features, ±0.25 mm or DIN 16901 class 130 on larger ones) and keep critical fits on machined inserts.
10. Inserts and overmoulding
Threaded inserts need a boss sized for the insert, a hole depth that leaves no witness on the opposite face, and enough surrounding wall to resist pull-out. Overmoulded grips need a mechanical key — a dovetail or through-holes — not just adhesion.
11. Text, logos and dates
Engraved text should be at least 0.4 mm deep with a 0.25 mm minimum stroke and a 10° draft on the walls. Raised text is easier to polish; engraved text holds dirt. Date stamps belong on a replaceable insert.
12. Resin choice and its consequences
Glass-filled grades buy stiffness and cost tool life. Flame-retardant grades can be corrosive. Transparent grades punish any flow hesitation with a visible line. If the resin is fixed by a safety certification, say so early — it constrains the gate and the tool steel.
Most DFM findings are not design failures, they are communication gaps. A 1.5 mm wall with a 3 mm boss is fine if the cosmetic face is hidden — and unacceptable if it is the front of a medical device.
How we run the review
We return the marked-up STEP file, a short written list ordered by cost impact, and two numbers: the price as submitted, and the price after the changes we recommend. You decide. Most of the time the second number is 15–40% lower and the tool arrives a week earlier.
Send a STEP or Parasolid plus the resin and the annual volume. If the part does not exist yet, we can also review a concept model before you commit to a design freeze.